Print parameters

Below we detail the recommended print guidelines that must be taken into account when printing with Recreus filaments to obtain the best possible quality and result. Remember that each printer is unique and it may sometimes be necessary to adjust the settings for best results.

Printing temperature

Print speed

Retraction distance

Retraction speed

Bed temperature

TDS & MSDS

Print Profiles

215ºC - 225°C

20-40 mm/s

2,5-6 mm

25-30 mm/s

Not required

215ºC - 235°C

20-40 mm/s

2,5-6 mm

35-50 mm/s

Not required

215ºC - 250°C

20-60 mm/s

4- 6 mm

40 mm/s

Not required

215ºC - 250°C

20-70 mm/s

3,5-6 mm

Direct Drive: 40-70 mm/s at a distance of 3.5 mm | Bowden: 40 mm/s at a distance of 6.5 mm

Not required

220ºC - 235°C

20-60 mm/s

2-3 mm

40 mm/s

50°C - 60°C

245ºC - 250°C

20 mm/s

2-3 mm

40 mm/s

50°C - 60°C

215ºC - 250ºC

26-60 mm/s

4-6 mm

40 mm/s

Not required

Filaflex SEBS

240ºC - 260ºC

20-40 mm/s

2-3 mm

40-60 mm/s

50°C - 60°C

245ºC - 255ºC

20-40 mm/s

2,5-6 mm

35-50 mm/s

Not required

230°C

40 mm/s

3,2 mm (direct extrusion)

6 mm (bowden type extrusion)

40 mm/s (direct extrusion)

25 mm/s (bowden type extrusion)

40°C once the 'primer' has been applied and after letting it dry for 5'.

240ºC - 260ºC

30-60 mm/s

2-3 mm

25-50 mm/s

40ºC once our primer is applied and 80ºC with other primers.

230ºC - 260°C

15-100 mm/s

3,5-6,5 mm

25-100 mm/s

40°C - 70°C

245ºC - 260°C

40-60 mm/s

1-2 mm

20-50 mm/s

70°C

215ºC - 225°C

20-100 mm/s

3,5-6,5 mm

20-160 mm/s

40ºC - 60°C

215ºC - 225°C

20-100 mm/s

3,5-6,5 mm

20-160 mm/s

40ºC - 60°C

240ºC - 260ºC

40-50 mm/s

2-3 mm

40-60 mm/s

60ºC

Additional recommendations:

It is recommended to dry the filament for 2 hours at 45-50°C in a conventional oven and with activated air circulation for optimal results.